EN 10083-3 Â |Â EN 10250-3 Â |Â Quenched and Tempered Engineering Steel
A nickel-chromium-molybdenum alloy designed for heavy shafts, gears and forgings that need high strength, real toughness through the section, and predictable behavior after oil quenching and tempering.
What is 34CrNiMo6 Steel?
34CrNiMo6 is a quenched and tempered alloy engineering steel, registered under material number 1.6582. It is standardized in EN 10083-3 for bar products and in EN 10250-3 for open-die steel forgings.
The chemical composition of this steel primarily consists of approximately 1.5% nickel, 1.5% chromium, and 0.25% molybdenum, with a carbon content close to 0.34%.Nickel lifts toughness and hardenability, chromium supports hardenability and surface strength, and molybdenum helps the steel resist softening during tempering.The result is 34CrNiMo6 steel that reaches 900 to 1200 N/mm2 tensile strength in common engineering sections while keeping useful impact values, even at low temperatures.
Chemical Composition
| Grade | C | Mn | P | S | Si | Cr | Ni | Mo |
| 34CrNiMo6/1.6582 | 0.30-0.38 | 0.50-0.80 | ≤0.025 | ≤0.035 | ≤0.4 | 1.3-1.7 | 1.3-1.7 | 0.15-0.3 |
Its strongest selling point is deep hardenability. On large round sections, the core hardens close to the surface rather than turning soft, which is why wind turbine main shafts and heavy transmission parts are so often specified in this grade.
However,34CrNiMo6 has only ordinary atmospheric corrosion resistance and will rust without paint, oil or another surface treatment. Weldability is limited because the alloy is sensitive to hardening and cracking in the heat-affected zone. It is also susceptible to temper embrittlement and to hydrogen flakes in large sections, both of which are controlled through correct heat treatment and verified testing rather than left to chance.
Where is 34CrNiMo6 Steel Used?
34CrNiMo6 steel is normally chosen for large, safety-relevant parts that carry repeated or shock loads rather than for simple brackets. Typical parts include:
34CrNiMo6 Steel Heat Treatment Basics
For 34CrNiMo6 steel, once the chemistry and section are fixed,the tempering temperature becomes the only effective means of balancing strength and toughness.Within the 540–680 °C window, hardness falls by roughly 0.5–1 HRC per 10 °C, which means a 40 °C change moves a part from a 320 HB wear-resistant condition to a 270 HB toughness-oriented one. Additionally, if possible, avoid high-temperature tempering within the temperature range of 350–550 °C. 34CrNiMo6 steel is prone to temper embrittlement within this temperature range.
34CrNiMo6+QT Mechanical properties per EN 10083-3
The following values ​​represent the performance requirements for 34CrNiMo6 after quenching and tempering according to EN 10083-3 standard.Note how quickly the guaranteed strength falls as the section grows: this is not a defect of the grade, it is a statement about how deeply it hardens in a given quench.
| Section (mm) | Rm (MPa) | Re (MPa, min) | A (%, min) | Z (%, min) | KV2 (J, min) |
| ≤ 16 | 1,200–1,400 | 1,000 | 9 | 40 | By agreement |
| 16–40 | 1,100–1,300 | 900 | 10 | 45 | 45 |
| 40–100 | 1,000–1,200 | 800 | 11 | 50 | 45 |
| 100–160 | 900–1,100 | 700 | 12 | 55 | 45 |
| 160–250 | 800–950 | 600 | 13 | 55 | 45 |
34CrNiMo6+QT Mechanical properties per EN 10250-3
For open-die forgings to EN 10250-3 the structure of the requirement is different: strength levels are lower but impact is specified in both longitudinal and transverse directions, which is far more demanding than the bar table suggests.
| Thickness (mm) | Rm (MPa) | Re (MPa) | A (%, L / T) | KV2 (J, L / T) |
| ≤ 160 | ≥ 800 | ≥ 600 | 13 / 9 | 45 / 22 |
| 160–330 | ≥ 750 | ≥ 540 | 14 / 10 | 45 / 22 |
| 330–660 | ≥ 700 | ≥ 490 | 15 / 11 | 40 / 20 |
In practice, a well-controlled Ø200 mm forged and Q&T bar can reach roughly 900–950 MPa tensile with 700–750 MPa yield, 17–18 % elongation and Charpy values above 100 J, at a hardness of about 300 HB. Those are typical achieved values, not guaranteed minimums. That gap between typical and guaranteed is why the purchase order must state the specimen location, test temperature and acceptance level.
34CrNiMo6 Steel Machining & Welding
Machining
Where the process route allows, 34CrNiMo6 should be machined in either the annealed (+A) or normalized (+N) state.At 248 HB maximum in the annealed state the steel cuts cleanly with carbide tooling and conventional speeds; in the Q&T condition at 300 HB or more, expect reduced tool life, higher cutting forces and a greater risk of surface damage on interrupted cuts.
If quenching is performed after machining, allowance should be made to remove deformation and decarburization. For thin-walled or asymmetrical parts, stress relief treatment should be performed before finishing.
Welding
The data doesn’t lie. There’s no doubt that 34CrNiMo6 steel has poor weldability and should not be used in welded structures.
If welding is unavoidable, preheating to 200–300 °C should be planned, a low-hydrogen welding process should be used, and post-weld heat treatment should be performed to eliminate residual stress. The welding process should be validated beforehand, as unheated welds on thick sections are highly susceptible to cracking.
34CrNiMo6 Steel vs. Other Deeper-Hardening Grades
Buyers often ask a more specific question than “Is 34CrNiMo6 steel good?”: “Is it worth the price?” The answer depends on section size and loading character.
| Grade | Chemistry signature | Practical through-hardening | Toughness and fatigue | Relative cost |
| 42CrMo4 | 0.38–0.45 C, 0.9–1.2 Cr, 0.15–0.3 Mo, no Ni | Reliable to roughly Ø100–150 mm in oil | Adequate; falls off quickly in thick sections | Baseline |
| 36CrNiMo4 | 0.32–0.40 C, 0.9–1.2 Cr, 0.9–1.2 Ni | Roughly Ø150–200 mm | Better than 42CrMo4, less than 34CrNiMo6 | +10–20 % |
| 34CrNiMo6 | 0.30–0.38 C, 1.3–1.7 Cr, 1.3–1.7 Ni, 0.15–0.3 Mo | Roughly Ø250–300 mm with good oil quenching | Best balance of strength and impact in this group | +20–35 % |
| 30CrNiMo8 | 0.26–0.34 C, 1.8–2.2 Cr, 1.8–2.2 Ni | Beyond Ø300 mm | Highest hardenability; also highest embrittlement sensitivity | +35–50 % |
How to choose?
Choose 42CrMo4 when the section is under about 100 mm, the load is mainly bending or tension, and induction or nitriding hardening is available for the wear surfaces. It machines better and costs less.
Choose 34CrNiMo6 when the section exceeds 100 mm, when the part carries torque or reversing loads (shafts, crankshafts, gears), when specified strength is above 1,000 MPa with impact requirements attached, or when the design cannot tolerate a soft core.
Choose 30CrNiMo8 only when a Jominy curve or section test proves 34CrNiMo6 cannot reach the required core properties.
Frequently Asked Questions
Top FAQs for engineers and buyers choosing 34CrNiMo6 alloy steel. Can’t find your question? Reach out to our technical support team anytime.
Request a Quote for 34CrNiMo6
- Dimensions and ruling section
- Delivery condition (+A, +QT, bright)Â Â
- Required strength and hardnessÂ
- Charpy test temperature (room, -20 or -40 °C) Â
- Ultrasonic testing levelÂ
- Quantity and destination port